From: "John Fisher" racer577 at citystar.com
I have used the 3.2 oz satin weave on 7 boats now. The first was a single layer and now that hull is 4 or 5 years olds it is showing wear and tear. I went to using 2 layers to help with durability and to have more material for sanding. Another thing I like about the cloth is that is drapes very nicely and easily will cover the hull with one pc. On my 10Rs I have used 2 yards folded in half to do the hull. On the star I was concerned that it would be too wide for a single yard. I ended up with more than enough material so I cut it on the diagonal.
The glassing starts by laying the glass over the hull. Then I smooth it out so there are no wrinkles. This may take a couple of min. Then I repeat with the next layer. Once the glass is smooth, time for epoxy. I used the 209/105 west systems combination. I used about 10 pumps of material.
I start applying resin to the middle of the bottom with a cheap paint brush. Then I work my way out to the edges of the bottom. Next I do the sides. You need to use lots of resin and dont pull too much or you will pucker the cloth. Once everything is wetted out I go back with a squigee and remove the excess resin. Dont get to carried away or the cloth will go dry again. If in doubt of how this should look practice on a spare block of wood first to get a feel for how the cloth looks as you take out resin.
I did the glassing at about 8 pm and with the 105/209 the resin is still green at 7 am the next morning. When green the glass can be trimmed with a #11 blade in a hobby knife. Then wait another day or two until sanding for full cure. I dont like to do much sanding, instead I try and do most of my fairing by using a thick primer and sanding most of it off between coats. For a clear boat I use polyurethane for a top coat.
I have used the 3.2 oz satin weave on 7 boats now. The first was a single layer and now that hull is 4 or 5 years olds it is showing wear and tear. I went to using 2 layers to help with durability and to have more material for sanding. Another thing I like about the cloth is that is drapes very nicely and easily will cover the hull with one pc. On my 10Rs I have used 2 yards folded in half to do the hull. On the star I was concerned that it would be too wide for a single yard. I ended up with more than enough material so I cut it on the diagonal.
The glassing starts by laying the glass over the hull. Then I smooth it out so there are no wrinkles. This may take a couple of min. Then I repeat with the next layer. Once the glass is smooth, time for epoxy. I used the 209/105 west systems combination. I used about 10 pumps of material.
I start applying resin to the middle of the bottom with a cheap paint brush. Then I work my way out to the edges of the bottom. Next I do the sides. You need to use lots of resin and dont pull too much or you will pucker the cloth. Once everything is wetted out I go back with a squigee and remove the excess resin. Dont get to carried away or the cloth will go dry again. If in doubt of how this should look practice on a spare block of wood first to get a feel for how the cloth looks as you take out resin.
I did the glassing at about 8 pm and with the 105/209 the resin is still green at 7 am the next morning. When green the glass can be trimmed with a #11 blade in a hobby knife. Then wait another day or two until sanding for full cure. I dont like to do much sanding, instead I try and do most of my fairing by using a thick primer and sanding most of it off between coats. For a clear boat I use polyurethane for a top coat.
0 komentar:
Posting Komentar